Borski, Justin
2004-08-09
William Lanford-Crick
2004-08-10
Paul Monaghan
LOR stripping while protecting Al
William Lanford-Crick
2004-08-09
We've never had trouble with the Acetone; this may be because we have baked
the LOR at 190 degrees.  I am told that acetone can cause some precipitate
in un-baked LOR but we have never experienced any trouble.

The kind folks at Microchem -- which supplies the LOR -- have suggested NMP
also, but warned that I should keep it as dry as possible to avoid etching
the aluminum.  We have a lab which has very poor humidity control--any
thoughts on how to prevent the bottle of NMP from absorbing moisture from
the air?  Or do you think this won't be a problem?

Thanks!
Bill

-----Original Message-----
From: [email protected]
[mailto:[email protected]]On Behalf Of Borski, Justin
Sent: Monday, August 09, 2004 8:14 AM
To: 'General MEMS discussion'
Subject: RE: [mems-talk] LOR stripping while protecting Al


Bill,

Usually, using acetone with LOR is a bad idea, if fact, I believe the vendor
will tell you that LOR and acetone are incompatible?

You should be able to lift off the film using NMP at 50 to 70 degrees C, and
that will strip the LOR material as well during the same operation.

-Justin

-----Original Message-----
From: William Lanford-Crick [mailto:[email protected]]
Sent: Sunday, August 08, 2004 5:30 PM
To: General MEMS discussion
Subject: [mems-talk] LOR stripping while protecting Al


Hi,
I've seen previous posts regarding the attack of Aluminum by common
developers.  I am using a bilayer resist for lift-off which is S1813 on
LOR-5B.  I need a chemical that can strip the LOR-5B without damaging the
Aluminum.

After metal deposition (which includes Al), I do the lift-off with Acetone
which works just fine.  Now I need to strip the LOR-5B.  I can use the 319
developer to etch LOR-5B but it is TMAH-based and thus etches the Aluminum.
Typically, I have a very thick edge-bead of LOR-5B which requires several
minutes of soaking in 319 dev. to remove.  This seems to really degrade the
Aluminum layer.

What can use I use to strip LOR-5B without damaging the aluminum layer?
Will NMP attack the aluminum?
Thanks!

Bill

_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/

**********************AMS CONFIDENTIAL AND PROPRIETARY
INFORMATION*****************************
This e-mail communication and any attachments are confidential and intended
only for the use of the designated recipients named above.


_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Mentor Graphics Corporation
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics