MEMSnet Home: MEMS-Talk: Dimples in SU-8 film
Dimples in SU-8 film
2007-03-20
Yue Mun Pun, Jeffrey
2007-03-20
Peng Li (Paul)
2007-03-20
Yue Mun Pun, Jeffrey
2007-03-20
Gareth Jenkins
2007-03-21
Yue Mun Pun, Jeffrey
PhotoResist - higher Glass transition temperature!!
2007-04-05
madhav rao
2007-03-20
Bill Moffat
Dimples in SU-8 film
Bill Moffat
2007-03-20
The dehydration bake is too short. To achieve dehydration in our vacuum vapor
primers we use 150 degrees C, 3 purges of hot Nitrogen and vacuum to 10 Torr.
Followed by a vacuum of 1 Torr.  At 1 Torr water boils at -20 degrees C.  Bil
Moffat

________________________________

From: [email protected] on behalf of Yue Mun Pun, Jeffrey
Sent: Tue 3/20/2007 1:55 AM
To: [email protected]
Subject: [mems-talk] Dimples in SU-8 film



Hi,
I am trying to coat 2-3 layers of SU-8 2050.  My process is aas follows:

1.  Dehydration bake SiO2 wfr at 120'C for 2mins
2.  Spin coat SU-8 2050 at 500rpm and ramp up to 3000rpm for 30sec.
3.  Soft bake the first layer at 65'C for 3mins (ramped from 50'C to 65'C and
hold for 3mins)
4.  Return wafer to spin coat another layer at the same conditions stated in 2.
5.  Soft bake wafer at 65'C for 5mins and ramp to 95'C for 20mins, since the
layers now have a nominal thickness of 100 microns.

I noticed that while baking at 95'C the SU-8 film developed dimples.  These may
or may not be an issue for my process, but they are cosmetically ugly.  Can
anyone tell me how do I solve this dimple issue?
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics
Addison Engineering
Harrick Plasma, Inc.