Is three is differences between BOE and HF solution (10-48%) for etching native oxide layer?
2008-11-12
Moshe
2008-11-13
Mantavya Sinha
2008-11-13
James Paul Grant
2008-11-14
汪飞
2008-11-14
James Paul Grant
2008-11-14
Christopher Tan
Is three is differences between BOE and HF solution (10-48%) for etching native oxide layer?
Christopher Tan
2008-11-14
I think James' point was not to imply that BOE is not-isotropic, but
that since BOE etches at a slower rate, it is easier to time and control
the undercut.

More importantly, if one wants to simply strip the oxide layer without
features and without caring about the surface smoothness, then obviously
a higher concentration would work quickly and very well. However, if one
wants to maintain a smooth Si surface without damaging the original
flatness of the wafer (such as for hydrophobic Si fusion bonding), one
should choose a much lower concentration of HF, such as diluted HF (DHF,
~1-6% HF in H2O) or 6:1, 10:1 or 50:1 BOE. High concentrations of HF
will damage the atomic flatness of the wafer.

Christopher Tan

汪飞 wrote:
> Dear James,
>
> "Obviously HF etching is isotropic (etches in all directions) so to reduce
> the undercut of patterned features one should choose an BOE concentration
> and etch time accordingly."
>
> I think BOE etching is also isotropic. So, why do you think it can help with
> better undercut profile?
>
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
Mentor Graphics Corporation
University Wafer
Process Variations in Microsystems Manufacturing