MEMSnet Home: MEMS-Talk: Re: Low stress SiN layer
Re: Low stress SiN layer
1995-11-15
Mark D. Walters
1995-11-15
[email protected]
Re: Low stress SiN layer
Mark D. Walters
1995-11-15
We have had a lot of experience depositing low-stress silicon nitride. The
nitride is deposited at 825 C using LPCVD. In order to get low-stress, the film
is made a little silicon-rich, which results in an index of 2.2. We garauntee a
stress of less than 100 MPa (Tensile), with typical values less than 50 MPa.

We could also grow (or deposit) the oxide for you as well, although we would
need to perform a test run to get the oxidation rate on <110> wafers.

If you would be interested in using our services, or would like to discuss our
capabilities further, feel free to contact me by phone or e-mail.
_____________________________________________________________________________
Mark D. Walters  ([email protected])
MEMS Technology Applications Center
MCNC
Research Triangle Park, NC  27709

Phone: (919) 248-1864
_____________________________________________________________________________


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Mentor Graphics Corporation
MEMS Technology Review
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing