MEMSnet Home: MEMS-Talk: Si3N4 with PECVD
Si3N4 with PECVD
2002-02-08
Zeila Zanolli
2002-02-08
Roger Shile
Si3N4 with PECVD
Roger Shile
2002-02-08
PEVCD generally does not produce Stoichometric Si3N4, but a variable
composition often denoted SixNyHz, or simply SiN.  When Texas Instruments
started using this stuff for IC passification in the mid '70, the corporate
buzz was "Sin is in".  Hydrogen content can be 20% or more.

If you use ammonia and silane in a ratio of ~6:1 at 380 degC in a PWS Coyote
you should get SiN with a refractive index of ~2.0, which is typical of Si3N4
produced by thermal LPCVD.  However this is a silicon rich material.  If you
use a higher ammonia to silane ratio you should be able to synthisize a
material with a Si to N ratio of 3:4, but the refractive index will probably
be low due to the hydrogen content.

You may have trouble with excessive stress and poor uniformity using 2% silane
in N2.  I would expect better results using pure silane and ammonia.  Yea its
dangerous stuff, maybe 10% would work.

>>> [email protected] 02/08/02 10:32AM >>>
Hi,
I'm trying to have Si_3 N_4 using a PECVD sistem.
I have at my disposal SiH_4 (Silane) (2% of SiH_4 in N_2) and N_2 and
i'm looking for a recipe to get Si_3 N_4.
Can someone give me some suggestion about the power, the temperature and
the ratios of Silane and Nitrogen?
Thanks a lot,
Zeila

[demime 0.98e removed an attachment of type text/x-vcard which had a name of
zanolli.vcf]
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
The Branford Group
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing