MEMSnet Home: MEMS-Talk: thick photoresist development
thick photoresist development
2004-02-16
Qing Yao
2004-02-16
Isaac Wing Tak Chan
2004-02-16
[email protected]
2004-02-16
[email protected]
2004-02-17
Gary
2004-02-17
Brubaker Chad
2004-02-17
Kevin
2004-02-18
Brubaker Chad
2004-02-18
Bill Moffat
thick photoresist development
Bill Moffat
2004-02-18
Qing,
     The total answer is to use image reversal.  I have experience with up to 30
micron thick resist, I am sure and will do tests with you to establish that 50
microns is O.K.  Think positive resist.  Reverse polarity mask.  Do the first
exposure which establishes the slope of the exposed area.  Then reverse, a warm
ammonia process that neutralizes the exposed resist.  Then flood expose and the
amount of flood expose determines the slope of the finished image.  Think of
going from a negative angle, through a vertical wall to a positive overhang just
by controlling the flood exposure.  Contact me directly for a number of
technical papers and how to do free tests.  Bill Moffat

-----Original Message-----
From: Qing Yao [mailto:[email protected]]
Sent: Monday, February 16, 2004 9:19 AM
To: MEMS-talk
Subject: [mems-talk] thick photoresist development


Hi,

I have difficulty in patterning thick photoresist. The following is what I did:

1> coat a 4" Si wafer with 5 layers of AZ4620 using a spinner. The thickness of
each layer is about 10 microns and the total thickness of PR is about 50
microns. Bake the wafer at 110 degree centigrade for 1 min. after the deposition
of each single layer.

2> print the image pattern on a transparency (emulsion down) using a 5080-dpi
laser printer. put the transparency mask on top of the PR layer and put a 4"
quartz plate on top of the mask. Then do Fusion Flood exposure. the dose is
about 3300 mJ/cm2. Lots of bubbles are generated during the exposure process.

3> use 1:4 AZ400K to develop the PR for about 9 minutes.

I used both optical microscope and surface profilometer to measure the side
wall. The slope angle is about 50 degrees.

However, I need the slope angle to be close to 90 degrees (at least larger than
80 degrees) so that it is almost perpendicular to the substrate. What can I do
to achieve it? Would you please give me any suggestions?

by the way, the thick photoresist layer is sort of mold (for electroless plating
of Ni on Si substrate).




Best Regards,


Qing Yao
___________________
M&IE @ UIUC
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Process Variations in Microsystems Manufacturing
Nano-Master, Inc.
MEMS Technology Review