HF solution releasing the SOI
2004-07-24
[email protected]
2004-07-26
Karin Buchholz
2004-07-25
Phillipe Tabada
HF solution releasing the SOI
Phillipe Tabada
2004-07-25
Hi Weidong,

   You shouldn't have a problem with the aspect ratio you have given.
Sometimes after a DRIE etch you might have a polymer residue preventing you
from etching the oxide underneath.  An oxygen plasma can normally remove
this polymer.  One way of determining where in your structure you still have
oxide is by using a microscope with an IR camera.

Phil Tabada


>From: 
>Reply-To: General MEMS discussion 
>To: [email protected]
>Subject: [mems-talk] HF solution releasing the SOI
>Date: Sat, 24 Jul 2004 10:12:42 +0800
>
>Dear colleges,
>      I use 80um thick device layer SOI wafer to fabricate a MEMS structure
>with DRIE. The box layer is 1.2um thick.The trenches in the structure is
>80um deep and 5um wide.When I release the structure with HF solution, I
>find it can't be released after many hours!what is the problem? The
>depth/width ratio is too high?
>Thanks for your possible help!
>                                                                Weidong
>Shen
>                                                       Zhejiang
>University,Hangzhou,P.R.China
>
>_________________________________________________________________
>Ãâ·ÑÏÂÔØ MSN Explorer:   http://explorer.msn.com/lccn
>
>_______________________________________________
>[email protected] mailing list: to unsubscribe or change your list
>options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>Hosted by the MEMS Exchange, providers of MEMS processing services.
>Visit us at http://www.memsnet.org/

_________________________________________________________________
MSN Toolbar provides one-click access to Hotmail from any Web page – FREE
download! http://toolbar.msn.click-url.com/go/onm00200413ave/direct/01/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Mentor Graphics Corporation
University Wafer
MEMStaff Inc.
Process Variations in Microsystems Manufacturing