Integrating a thick dielectric layer surrounding suspended silicon nitride membranes
2008-06-02
Ken Healy
2008-06-02
Roger Shile
2008-06-02
Paul Sunal
2008-06-03
Michael D Martin
2008-06-03
Ken Healy
2008-06-03
Roger Shile
Integrating a thick dielectric layer surrounding suspended silicon nitride membranes
Paul Sunal
2008-06-02
Ken,

We can easily grow >10 um of thermal oxide, but the real trick is the
final release of the nitride diaphragm.  If you have very large
diaphragms, they may not survive once the anisotropic silicon etch is
finished and it's free-standing.  The stress in this thick of an oxide
may shatter if the diaphragm is large.

You are correct by assuming a plasma etch will not work since the
nitride does not serve as an etch stop and that you have such a thin
layer.  This means you are limited to HF, either wet or vapor etching.
Five microns of thermal oxide is not an easy thing to etch either.  This
will take some time to do.

In both cases you'll have undercutting of the membrane, which will make
the diaphragm larger than you planned.  The curved oxide wall and larger
diaphragm will affect your capacitance as well.

Best of luck,

Paul

> Hello,
>
> I'd like to ask for advice on how best to modify the standard
> procedure for fabricating suspended silicon nitride membranes to
> incorporate a thick dielectric layer (>=5um).
>
> The aim is to reduce the capacitance from the top to the bottom of the
> chip supporting the membrane, as it will be used to separate two
> chambers of conductive fluid. The capacitance with standard membranes
> is very high since the thickest dielectric layer is the thin silicon
> nitride (50-100 nm in my case).
>
> Reducing the fluid contact area will reduce the capacitance, but the
> microfluidics required to achieve an equivalent reduction in
> capacitance appears more complicated than adding a dielectric layer.
>
> (The particular application I'm working on is nanopore-based DNA
> analysis, where the noise level scales with capacitance. For
> background info see http://eleceng.ucc.ie/nanopore/)
>
>
> The best process I have come up with so far is as follows, but it's
> still significantly more complicated than the standard procedure for
> silicon nitride membrane fabrication. See the diagram below for
> reference.
>
>
> membrane nitride
> ======================================================================
> dielectric oxide               |        |
> --------------------------------        ------------------------------
>                               /          \
>                              /            \
> silicon                     /              \
>                            /                \
>                           /                  \
> --------------------------                    ------------------------
> mask oxide               |                    |
> ==========================                    ========================
> mask nitride
>
>
> 1. Grow 5 um thermal oxide on 100 silicon wafers (on both sides to avoid
> wafer bow due to stress)
>
> 2. Grow 50-100 nm low-stress silicon nitride on top of the oxide
>
> 3. Follow the standard membrane fabrication procedure to define openings
> in the mask nitride layer.
>
> 4. Anisotropically etch the mask oxide layer with CHF3/O2 plasma,
> protecting the silicon nitride with photoresist.
>
> 5.KOH-etch the silicon following the standard membrane fabrication
> procedure.
>
> 6. Finally, etch the exposed dielectric oxide with CHF3/O2, protecting
> the membrane silicon nitride with photoresist.
>
> 7. Remove any fluoropolymer residue resulting from the CHF3/O2 etch
> with oxygen
> plasma.
>
>
> Any suggestions would be greatly appreciated.
>
> Best regards,
>
> Ken Healy
>
> Dept of Physics and Astronomy
> University of Pennsylvania

--
==================================
Paul Sunal, PhD
Senior MEMS Engineer

MEMS and Nanotechnology Exchange / CNRI
1895 Preston White Drive
Suite #100
Reston, VA  20191

Tel: 703.262.5323
Fax: 703.262.5367
==================================

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing
MEMStaff Inc.
Mentor Graphics Corporation