MEMSnet Home: MEMS-Talk: Deposition of Chromium and Platinum
Deposition of Chromium and Platinum
2009-01-19
Yinyan Gong
2009-01-19
Ruiz, Marcos Daniel (SENCOE)
2009-01-20
Yinyan Gong
2009-01-20
Ruiz, Marcos Daniel (SENCOE)
2009-01-19
John Hilton
2009-01-19
Edward Sebesta
2009-01-20
Yinyan Gong
2009-01-20
Edward Sebesta
2009-01-22
Evelyn B
2009-01-20
Jie Zou
Deposition of Chromium and Platinum
Yinyan Gong
2009-01-19
Dear All,

I have a hard time to deposit Chromium (50nm) followed by Platinum
(100nm) using a e-beam evaporator. After lift-off (using 1165), some
areas of the metal layer will peel off and the rest part has very rough
surface. I note that during deposition of Pt, the temperatures is quite
high and I have to interrupt the deposition when the temperature reaches
90C and let the system cool down before depositing again. Any
suggestions will be appreciated.

Best regards

Yinyan
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Mentor Graphics Corporation
Process Variations in Microsystems Manufacturing
Nano-Master, Inc.