High contrast photoresist for interference lithography
2013-01-15
Justin Hannigan
2013-01-15
Daniel Figura
2013-01-16
Justin Hannigan
2013-01-16
Andrew Sarangan
2013-01-16
Justin Hannigan
High contrast photoresist for interference lithography
Daniel Figura
2013-01-15
Hello Justin,

I think you can use most of the broadband photo resists like AZ 15xx, AZ
33xx, AZ MIR 701, Shiply S18xx, JSR ....

Some materials will be easier (faster, small sample) to get then other.

High resolution is relative - what L/S resolution do you need? Limiting
factor can be photo resist contrast but very often exposure system.

Some time ago I made a list of commercially available UV photo resists
http://www.smartfabgroup.com/photoresists.php have a look.


With best regards,

Daniel



Daniel Figura

smartfabgroupT Company

process consulting . data processing . fab software

Phone: +421 944 45 26 86

E-mail: [email protected], Web: www.smartfabgroup.com



Disclaimer notice: The information contained in this message and any
attachments is intended only for the personal and confidential use of the
designated recipient(s) named above. If you are not the intended recipient
of this message you are hereby notified that any review, disseminitation,
distribution or copying of this message is strictly prohibited. If you have
received this message by error, please notify the sender immediately.



-----Original Message-----
From: [email protected]
[mailto:[email protected]] On
Behalf Of Justin Hannigan
Sent: Tuesday, January 15, 2013 19:02
To: [email protected]
Subject: [mems-talk] High contrast photoresist for interference lithography

Hi,

I am looking for a high-contrast, high-resolution photoresist to use for
interference lithography.  Our source is a HeCd laser operating at the
442 nm line.  Ultimately, we would like to use the resist as an etch
mask, so resistance to fluorine-based chemistry would be beneficial but
isn't strictly necessary.

I have been working with ma-p 1205 but I have difficulty getting steep
sidewalls.  I have gotten some good prints using a diluted SPR 220 in
the past, but I have had difficulty getting consistent dilutions so I
would prefer a commercial pre-mixed product.

As I understand it, the high-resolution requirement requires a low
viscosity resist that will produce a thin layer when spin coated. (Since
we are doing an interference lithography we don't have depth of focus
issues, but there's still a limit on the aspect ratio for the lines that
limits the resist thickness to less than a micron.)

To summarize, I'm looking for a photoresist that has the following
properties:
1) Sensitive at 442 nm (g-line resists seem fine)
2) Low viscosity; film thickness less than 1 micron
3) High contrast (large change in development rate when exposed)

Can anyone recommend a suitable product for this?

Justin

--
Justin M. Hannigan, Ph.D.
Process Development Engineer
LightSmyth Technologies,Inc.
875 Wilson St, Unit C
Eugene, OR 97402
Tel: 541-431-0026
www.lightsmyth.com


!DSPAM:50f5999e205381938014717!


_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk

_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics
Nano-Master, Inc.
MEMStaff Inc.