MEMSnet Home: MEMS-Talk: About difficulty in photoresist development (if using HMDS as adhesion layer)
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-23
Mehmet Yilmaz
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
Bill Moffat
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
André Bödecker
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-24
James Guenes
2015-09-25
Liang Zhao
2015-09-25
Orozaliev Ajymurat Nurdinovich
2015-09-29
Mehmet Yilmaz
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-25
Mohammad Yusuf Mulla
About difficulty in photoresist development (if using HMDS as adhesion layer)
2015-09-29
Andrew Sarangan
2015-09-30
Mehmet Yilmaz
2015-10-04
Andrew Sarangan
2016-01-04
Mehmet Yilmaz
2016-01-04
조명래
2016-01-04
ozgur celik
2016-01-05
André Bödecker
2015-09-25
Brian Baker
About difficulty in photoresist development (if using HMDS as adhesion layer)
Mehmet Yilmaz
2015-09-29
Dear all,
Thanks for all of your replies. I could not reply earlier. I am sorry about
that.

@ Bill Moffat, I am using HMDS (UN3286) from TECHNIC FRANCE. I use HMDS
spinning rather than Vacuum Prime Oven. We do not Vacuum Prime Oven here.
What I realized is, spinning HMDS is not recommended by the vendor... But,
I do not have any other way to coat HMDS in our facilities.

@ André Bödecker, James Guenes, Liang Zhao, I looked at the datasheet. It
does not recommend spinning HMDS. I was not aware of that due to my earlier
experience with HMDS at other cleanroom facilities...
http://www.microchemicals.com/products/adhesion_promotion/hmds.html

@ Mohammad Yusuf Mulla, thanks for the recipe.

@ Orozaliev Ajymurat Nurdinovich, thanks for the information.

I have a quartz substrate that I need to work with. I will try to clean it
at first, and then skip HMDS adhesion layer spinning, since it is not
recommended by the vendor. I will let you know once I have a run-path for
this problem.

Regards,

Mehmet

On Fri, Sep 25, 2015 at 11:29 AM, Orozaliev Ajymurat Nurdinovich <
[email protected]> wrote:

> Mehmet,
>
> HMDS shouldn't have an effect on development time since it is only a single
> layer.
> I would check the baking temperature and time.
> Also, if you are using the YES oven, try to coat the resist after the wafer
> temperature reduces to room temperature.
>
> I sometimes do not use HMDS at all. Instead I bake the wafer at 200 C for 5
> mins and after it cools down I immediately coat my resist and I do not have
> an adhesion problem.
>
> good luck,
> Ajy
>
>
>
> On Thu, Sep 24, 2015 at 4:21 PM, James Guenes 
> wrote:
>
> > Mehmet,
> > your problem is the combination of thickness combined with HDMS.
> >
> > Potential Solution:
> > Have a list of the properties of the HDMS and find a compound that will
> not
> > insist to stick to the matter for a very long time, which means you have
> to
> > conduct experiments with various solutions under tightly controlled
> > environments.
> >
> > All the best of luck to you, I hope that my observation was a little
> > insightful,
> >
> > On Mon, Sep 21, 2015 at 5:24 AM, Mehmet Yilmaz  >
> > wrote:
> >
> > > Dear mems-talk community,
> > > If I use HMDS as adhesion layer, I am having a problem with the
> > development
> > > of a photoresist called AZ4562 (about 10 micron thickness). In
> addition,
> > I
> > > am having the same development problem with AZ5214E (about 1.4 micron
> > > thickness).
> > >
> > > If I do not use HMDS, the development time is usually about 60 seconds,
> > or
> > > even less. However, if I use HMDS, the development time goes up to 45
> > > minutes (not seconds...) and still the development is not successful,
> but
> > > the resist is completely removed from some parts of the patterned areas
> > on
> > > the wafer.
> > >
> > > Also, I have seen this problem with different substrates such as
> Silicon,
> > > Quartz, and Pyrex.
> > >
> > > I am wondering what would be the reason for that? Is it possible that
> > HMDS
> > > is old, and out of date? Could that explain the problem? Or, do you
> have
> > > any other comments based on your own experience? Could you please
> > comment?
> > >
> > > I am looking forward to your replies.
> > >
> > > Thanks in advance,
> > >
> > > Mehmet
> > >
> > > Mechanical Engineer
> > > _______________________________________________
> > > Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> > > provider of MEMS and Nanotechnology design and fabrication services.
> > > Visit us at http://www.mems-exchange.org
> > >
> > > Want to advertise to this community?  See http://www.memsnet.org
> > >
> > > To unsubscribe:
> > > http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> > >
> >
> >
> >
> > --
> > James Guenes
> > Electrical, Controls, Integration, Automation, Systems, Research,
> Reverse,
> > and Process Engineer
> > 513.482.9175 cell
> > Connect With Me on LinkedIn
> > <
> >
> https://www.linkedin.com/profile/public-profile-settings?trk=prof-edit-edit-
public_profile
> > >
> > ------------------------------
> > *The information in this email is intended only for the personal and
> > confidential use of the designated recipient above. If the reader of this
> > message is not the intended recipient or an agent responsible for
> > delivering it to the intended recipient, you are hereby notified that you
> > have received this document in error, and that any review, dissemination,
> > distribution or copying of the message is strictly prohibited. If you are
> > not the intended recipient, please contact the sender immediately by
> reply
> > e-mail and destroy all copies of the original message.*
> > _______________________________________________
> > Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> > provider of MEMS and Nanotechnology design and fabrication services.
> > Visit us at http://www.mems-exchange.org
> >
> > Want to advertise to this community?  See http://www.memsnet.org
> >
> > To unsubscribe:
> > http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> >
> _______________________________________________
> Hosted by the MEMS and Nanotechnology Exchange, the country's leading
> provider of MEMS and Nanotechnology design and fabrication services.
> Visit us at http://www.mems-exchange.org
>
> Want to advertise to this community?  See http://www.memsnet.org
>
> To unsubscribe:
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk
>
_______________________________________________
Hosted by the MEMS and Nanotechnology Exchange, the country's leading
provider of MEMS and Nanotechnology design and fabrication services.
Visit us at http://www.mems-exchange.org

Want to advertise to this community?  See http://www.memsnet.org

To unsubscribe:
http://mail.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Mentor Graphics Corporation
Tanner EDA by Mentor Graphics
Addison Engineering
Process Variations in Microsystems Manufacturing