MEMSnet Home: MEMS-Talk: KOH etching problem
KOH etching problem
2001-09-05
li shifeng
2001-09-12
Yahong Yao (2 parts)
spin photoresist after releasing the structure
2001-09-27
Yong Zhu
KOH etching problem
Yahong Yao
2001-09-12
Hi, Shifeng,

I think your Nitride film quality is not good.  I used 1000A nitride to etch
through a 4" wafer.  The Nitride was still very good after about 9 hours.
The KOH was 30% at 85C.

But I also encountered bad case in which the nitride had lots of blisters
after 30mins etch in KOH.  I suspect that the cleaning process was not
thorough before nitride was put on.  Further experiment is in progress.

Pls share me what you get.  Thanks.

Yahong


>From: "li shifeng" 
>To: [email protected]
>Subject: [mems-talk] KOH etching problem
>Date: Wed, 05 Sep 2001 20:39:31
>


_________________________________________________________________
Get your FREE download of MSN Explorer at http://explorer.msn.com/intl.asp
Hello to all, when i fabricate my device, i met one problem about KOH
etching.I deposited around 3500-4000A low stress LPCVD nitrid as KOH
etching through mask.I opened one window and then KOH etching.After five
to six hours, even 3500-4000A LPCVD nitrid was mostly stripped off.I do
not know the exact reason for this.i used 49% wt KOH 80deg c etching.I
know at this condition, nitrid etching rate is nearly zero.how come like
this? After that, i thought it over.it maybe the following reason. Even
i chose Low stress LPCVD nitrid, but the deposited time is still too
long,it is about 20 hours and the deposit temprature is high.so at the
last, the accumulted stress in nitrid is still high.when KOH etching, H2
bubble comes out.When bubble broken, suface tension will strip off high
stress nitrid. I amnot sure about this.some one has my similar
experiences.please confirm this for me. Thanks shifeng Li

------------------------------------------------------------------------
Get your FREE download of MSN Explorer at http://explorer.msn.com[1]
_______________________________________________ mems-talk mailing list
[email protected] To unsubscribe or change your list options, use:
http://fab.mems-exchange.org/mailman/listinfo/mems-talk
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics
MEMStaff Inc.
The Branford Group