MEMSnet Home: MEMS-Talk: Al oxide removal
Al oxide removal
2002-03-29
[email protected]
2002-03-29
[email protected]
2002-04-05
Jörn Koblitz
2002-04-09
[email protected]
Al oxide removal
[email protected]
2002-04-09
Try asking the foundary to do a short HF/PHO3, and an in-situ Ar(g) sputter
etch rior to
dep, if possible.

-----Original Message-----
From: Jvrn Koblitz [mailto:[email protected]]
Sent: 05 April 2002 14:49
To: [email protected]
Subject: RE: [mems-talk] Al oxide removal


Dear Barry,

The formation of a insulating layer (may be Al oxide, may be something
else) on your Al may be linked to the way you open the oxide pads. If
you use a wet BOE or dedicated pad etch, an Al hydroxide or
hydrofluoride layer can be formed. If you use HF gas, a quite stable Al
fluoride layer is formed. If RIE is applied, a fluoride layer may also
be formed depending on your process conditions. Also, you have to take
care about the possibility of electrochemical corrosion of the Al after
processing. This can happen, when there are other metals or higly doped
Si areas in contact to the Al and exposed to air, or if metalized wafers
are placed for too long time in humid air or rinsing baths. You see, it
can be a quite complex issue.

In case that you need further foundry services, let me know. We can also
do the job.

Best regards,

Joern Koblitz

******************************
Joern Koblitz
microFAB Bremen GmbH - the MEMS wafer foundry
Universitaetsallee 5
D-28359 Bremen, Germany
Phone: +49 421 24 100 0
Fax: +49 421 24 100 99
eMail: [email protected]
website: www.microfab.de
******************************

-----Original Message-----
From: [email protected] [mailto:[email protected]]
Posted At: Friday, March 29, 2002 6:08 PM
Posted To: MEMS-talk
Conversation: [mems-talk] Al oxide removal
Subject: [mems-talk] Al oxide removal


Dear MEMS coworkers,

We currently utilize foundry service to fabricate our MEMS platform, and
we
functionalize the platform by coating a proprietary material. The
existing
platform design calls for, fresh out of foundry, a SiO2 top layer with
contact openings to the underlying Al.

The issue we run into is that the exposed Al is easily oxidized and the
contact resistance varies from sample to sample. We have tried using
chemistry removing the aluminum oxide layer prior to functionalization.
Yet
the oxidation happens so rapidly that a  thin insulating oxide is formed
between sample transfer (in air), so we alleviated but not eliminated
the
reproducibility difficulty.

I appreciate any insights.

Regards,

Barry Chen
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/


***************************************************************************

This email and any attachments are confidential to the intended
recipient and may also be privileged. If you are not the intended
recipient please delete it from your system and notify the sender.
You should not copy it or use it for any purpose nor disclose or
distribute its contents to any other person.

***************************************************************************

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
Nano-Master, Inc.
Process Variations in Microsystems Manufacturing
The Branford Group