MEMSnet Home: MEMS-Talk: Cr/Au delamination
Cr/Au delamination
2002-04-09
Jiang Zhe
2002-04-09
shay kaplan
2002-04-09
Jiang Zhe
2002-04-09
Mike Pedersen
2002-04-09
adnan merhaba
2002-04-09
Atzmon Ofri
2002-04-09
[email protected]
2002-04-09
Maurice Norcott
2002-04-09
Henry Yang
2002-04-10
Henry Yang
Cr/Au delamination
Atzmon Ofri
2002-04-09
Dear Jiang Zhe

30 min in concentrated HF will attack the Cr regardless his thickness. From
my experience Cr will survive only 5-7 min in HF. Try to reduce the etch
time by holes (See Lucent Lambda mirrors).

Atzmon Ofri

-----Original Message-----
From: Jiang Zhe [mailto:[email protected]]
Sent: Tuesday, April 09, 2002 5:40 PM
To: [email protected]
Subject: [mems-talk] Cr/Au delamination


I have a 300A Cr/2500A Au delamination problem. Cr/Au

was deposited on p-type Si <100> wafer. Then it was
put

into concentrated HF and Cr/Au layer were peeled off

after 30 minutes. The pre-clean (RCA clean and a 2min

Ar plasma pre-etch) was well done before sputtering.

My question is, what's the possible reason of the

delamination? Any suggestion? Thanks!

Jiang
Yahoo! Tax Center - online filing with TurboTax
http://taxes.yahoo.com/
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing
The Branford Group