Pt on SiO2
2002-05-15
iog
2002-05-15
Mighty Platypus
2002-05-16
Helen Berney
Pt on SiO2
Mighty Platypus
2002-05-15
Hello Igor,
We use either Chrome or Titanium as an adhesion layer for Platinum. Ti has
a lower stress and can handle higher temperatures, while Cr is not
attacked by BOE. We deposit using E-beam evaporation.

We typically etch Pt with Aqua Regia. PR works well for patterning.

Jesse Fowler
  UCLA/MAE Dept., 420 Westwood Plaza, Room 37-129, ENGR IV
  Los Angeles, CA 90095-1597 | (310)825-3977
"Battery is safe if not provoked." -- _Batteries in a Portable World_
----- BEGIN GEEK CODE BLOCK -----
Version 3.1
GE/S$ d- s:- a- C+ UL P L++ E- W+ N+@ !o K++ w !O M !V PS+ PE++(-) Y
PGP-- t++@ 5++ X R+ !tv b++ DI+ D G e++/*>++++/* h---/* r+++ y+++
------ END GEEK CODE BLOCK ------


On Wed, 15 May 2002, iog wrote:

> Hello all,
>
> Who can tell if Pt has good adhesion to SiO2? And what can it be etched with?
>
> Thanks & Best regards,
>
> Igor
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.mems-exchange.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
Addison Engineering
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation