MEMSnet Home: MEMS-Talk: SiN passivation problem
SiN passivation problem
2002-06-05
Bill Moffat
2002-06-05
MM Farooqui
2002-06-05
BERAUER,FRANK (HP-Singapore,ex7)
2002-06-06
Bill Moffat
2002-06-15
TEL Klaus Beschorner
SiN passivation problem
Bill Moffat
2002-06-06
Hi,
   The compounds of HMDS were created inside the process chamber.  The process
works by delivering HMDS vapor to a plasma field that disassociates the HMDS.
It then redeposit down stream with all the differing compounds.  The result is
a sticky mess that can be as thick as you wish, and is hydrophobic.  The only
down side I know is the goop deposits every where and the interior of your
chamber gets sticky.  I don't know the age of the IBM patent but it is
definitely over 10 years old.  Let me know if I can help some more Bill
Moffat.

-----Original Message-----
From: MM Farooqui [mailto:[email protected]]
Sent: Wednesday, June 05, 2002 2:58 PM
To: [email protected]
Subject: RE: [mems-talk] SiN passivation problem


Bill

What are the compounds of HMDS that you deposited (which could be used on
aluminium metallization) "which remained hydrophobic for ever, removeable
with a simple eraser but difficult to clean" from your equipment ? Any
information will be highly appreciated.

regards

m.farooqui

> A possible answer.  IBM developed a process incorporating plasma and HMDS
> in the same system to deposit various compounds of HMDS.  It was a thick
> think many microns of sticky goop that was totally Hydrophobic.  The
> concept was for protection of Hybrid circuits in a submarine.  The part
> had to protected for ever against moisture but the material had to be
> easily removable.  I ran some experiments at that time combining one our
> plasma systems with a HMDS delivery system.  The thick goop was totally
> Hydrophobic, removable with a simple eraser, but if undisturbed remained
> hydrophobic for ever.  Down side the equipment I was using had the goop
> deposited every where and was difficult to clean.  Let me Know if I can
> help to find original IBM patents etc.  Bill Moffat
>
> -----Original Message-----
> From: Robert Dean [mailto:[email protected]]
> Sent: Wednesday, June 05, 2002 8:11 AM
> To: [email protected]
> Subject: [mems-talk] SiN passivation problem
>
>
> >Hello,
>
> I have a MEMS sensor that has aluminum traces covered with 0.4um of
> silicon-nitride, for passivation, that must operate in a moist-salty
> environment.  The part has failed, and I suspect that the moist-salty air
> has permeated through the SiN layer and damaged the aluminum traces
> underneath.  Any suggestions?
>
>
> Robert Dean
>
> Research Associate IV
> Center for Advanced Vehicle Electronics
> Auburn University
> 200 Broun Hall
> Auburn, AL 36849
>
> Voice: 334-844-1838
> Fax:   334-844-1898
> Email: [email protected]
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
MEMS Technology Review
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation