Sonbol Massoud-Ansari
1996-12-12
Osborn, Thor
boron diffusion
Osborn, Thor
1996-12-12
I have used spin-on dopants for boron diffusion in my doctoral thesis.
AlliedSignal's B-150 (Allied-Signal, Milpitas, CA)  formulation of
borazole polymer worked well for creating etch-stopped membranes of
silicon about 3.5 micron thick in EDP "F" solution.  The exact results
you get will depend on your furnace conditions.  I simulated the results
with SUPREM by assuming that the concentration of boron was at the solid
solubility limit on the surface at all times, and got good match between
simulation and actuals based on a 7*10^19 boron atom per cubic
centimeter requirement for etch survival.

The exact conditions I used were as follows:

Spin B-150 at 3000 rpm for 30 seconds

Furnace ramp up from 850 degrees C to 1200 degrees C over 40 minutes in
4 liter/min N2 and 100 cc/min O2 (3-inch wafers were used).

Hold at 1200 degrees C for 40 minutes.

Ramp down to 850 degrees C over 60 minutes in 4 liter/min O2

My furnace conditions were limited by my furnace and may not be optimal.

There is a further issue you should be aware of, which is that the
doping process leaves a surface film of high-boron concentration glass
that etches VERY slowly in 10:1 BHF.  It is much faster in 49% HF (about
one minute).

Further information can be found in my thesis:

"Development of a Mass Producible Lipid Bilayer Support Device" by Thor
Dane Osborn.  University of Washington (Seattle, WA)  1994.


I hope this is of some help to you.

Thor Osborn

 ----------
>>>From: Sonbol Massoud-Ansari
>>>To: [email protected]
>>>Subject: boron diffusion
>>>Date: Monday, December 09, 1996 9:12AM
>>>
>>>
>>>Dear MEMS researchers,
>>>
>>>I am trying to find some information about spin-on sources for deep boron
>>>diffusion (to be used as an etch stop for EDP etching).
>>>
>>>I would appreciate any information on commercial vendors & manufacturers
for
>>>the spin-on boron sources. In addition, if any one has any experience with
>>>using spin-on sources for deep boron diffusion, I would appreciate
>>>any information on the quality, performance, profile etc.
>>>
>>>In addition, I need to locate companies/labs that can do deep boron
>>>diffusion, using either liquid sources or spin-on sources, as a
>>>commerical service.
>>>
>>>Thank you,
>>>
>>> -Sonbol Massoud-Ansari
>>>
>>>
>>>


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
University Wafer
MEMS Technology Review
Process Variations in Microsystems Manufacturing