Hi Mike,

try 165g (NH4)2Ce(NO3)6 and 43 ml HClO4 in 1000ml water.

Antje

Michael Roper schrieb:

> Hello,
>
> I just ordered some chrome etchant from a commercial supplier, but it is going
> to take ~ 2 weeks to get here and I would like to have it fairly soon.  I've
> seen that HCl and H2O2 will etch chrome, and I was wondering if this mixture
> would also remove photoresist?  Does anyone know a homemade chrome etch
> solution that will not attack photoresist?  Thanks for any help you can give.
>
> Mike
> --
> Michael Roper
> University of Michigan
> Department of Chemistry
> 1500 N. University #4730
> Ann Arbor, MI 48108
> 734-615-4376
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
antje.vcf (text/x-vcard, 247 bytes)
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation
MEMS Technology Review