Can parylene resist the attack of KOH andTMAH?
Mighty Platypus
2002-11-29
Hello Li Gang:
My experience has been that a parylene coat will protect a wafer pretty
well in KOH. It isn't attacked, but it does peel. So, you really can't use
it for a mask. But, if it's all the way across the front, it'll probably
resist peeling.

Jesse Fowler
  UCLA/MAE Dept., 420 Westwood Plaza, Room 37-129, ENGR IV
  Los Angeles, CA 90095-1597 | (310)825-3977
"Never worry again about the quality of your random numbers!"
    -- Advertisement

On Thu, 28 Nov 2002, Gang Li wrote:

> Dear all,
>
> Can parylene be used to protect frontside of the wafers when
> you carry on etching trough the wafers from the backside?
> Any information will be appreciated greatly.
>
> Regards,
>
> Li Gang
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
>


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
Process Variations in Microsystems Manufacturing
The Branford Group
Harrick Plasma, Inc.