MEMSnet Home: MEMS-Talk: Re: Etching solutions
Re: Etching solutions
1997-07-23
jonathan d trumbull
1997-07-23
Shekhar Bhansali
1997-07-24
Mehmet Arik
Re: Etching solutions
jonathan d trumbull
1997-07-23
Michael,

To etch Ti you could use:

 Buffered HF (49%), Hydrogen Peroxide (30%), DI water in the ratios of 1:1:20

For gold, a popular recipe is:

 Potassium Iodide, Iodine, DI water in ratios (of mass) 4:1:30

--Jonathan